Installation Guides
Preparing your room, fitting engineered wood, herringbone and chevron, and a technical summary of BS 8201 for specifiers. Please share these with your fitter.
Figures marked (BS 8201) follow BS 8201:2011 Code of practice for installation of flooring of wood and wood-based panels. Other figures are ESB Flooring recommendations. Where the adhesive, underlay or heating manufacturer gives stricter instructions, follow theirs. If in doubt, call us on 020 8204 8555 before you start.
1. Preparing Your Room and Subfloor
Most flooring problems are caused by the room, not the floor. Please share this guide with your fitter.
Before your flooring arrives
- The building must be weathertight, with windows and external doors fitted.
- Plastering, screeding, tiling and painting must be finished and dry.
- Heating must be working. Underfloor heating must be commissioned first (see our Underfloor Heating Guide).
- The room should be at normal living conditions: 15–25°C and 45–65% relative humidity.
- Never store flooring in a garage, shed or damp area.
Acclimatisation
- Store packs flat and unopened in the room where they will be laid, raised off the floor.
- Allow at least 72 hours (longer for solid wood and wide boards).
Subfloor moisture
- Concrete and screed: below 65% RH measured with a hygrometer (BS 8201). Between 65% and 75%, use a damp-proof membrane approved by the adhesive maker. Above 75%, do not install.
- Plywood, OSB and floorboards: moisture content below 14%.
- Ask your fitter to record the readings and give you a copy.
Subfloor flatness
- No more than 3 mm under a 2 m straight edge (BS 8201). High spots ground down, low spots filled with levelling compound.
- The subfloor must be clean, sound and free of old adhesive and dust. Timber subfloors must be screwed down firmly with no movement.
Kitchens
Fit kitchen units before the floor where possible. A floating floor must never be fixed down by units or islands.
After fitting
- Protect the floor with breathable protection while other trades are working. Never tape protection to the floor.
- Keep the room at 15–25°C and 45–65% humidity all year. A humidifier may help in centrally heated homes in winter.
- Use felt pads under furniture and mats at outside doors.
2. Fitting Engineered Wood Flooring
Read with section 1. We recommend a professional fitter who uses a moisture meter.
Before you start
- Check the product, grade and colour against your order before opening packs.
- Inspect every board in daylight. Do not fit any board you are not happy with – set it aside and call us.
- Mix boards from at least three packs at a time.
- Allow 5–10% extra for cutting and waste.
Expansion gaps
Leave a gap around the whole room, and around pipes, door frames and fixed units: at least 10 mm, or 1.5 mm for every metre of floor width, whichever is greater. Use expansion profiles at doorways.
Fitting methods
- Glue-down (fully bonded) – best for wide boards, large areas and underfloor heating. Use a flexible, solvent-free wood flooring adhesive (MS polymer) and the trowel the adhesive maker specifies. Wait at least 24 hours before furniture.
- Secret nailing – over a sound timber subfloor. Fix through the tongue at 45°, every 200–300 mm, no closer than 50 mm to board ends.
- Floating – over a flat, dry subfloor with a suitable underlay and a damp-proof sheet over concrete. Maximum board width 220 mm and maximum 8 m in any direction without an expansion break. Never fix units through a floating floor.
Finishing
Fix skirting or beading to the wall, never to the floor. Keep a few spare boards for future repairs.
3. Fitting Herringbone and Chevron
Herringbone and chevron need accurate setting out. We recommend an experienced professional fitter. Read with sections 1 and 2.
- Wood herringbone and chevron must be glued down, never floated. (Laminate and click vinyl herringbone are floated – follow the instructions in the pack.)
- Many products have left (A) and right (B) blocks. Keep them separate.
- Allow 10–15% extra for cutting and waste.
- Subfloor moisture and flatness as section 1.
- Snap a centre line, dry-lay a few rows first to check the pattern and the cuts at the walls, and start against a square template or batten.
- Check the first rows are straight and square – errors at the start cannot be corrected later. Let the first rows set before building off them on concrete.
- Leave the same expansion gap as section 2 (minimum 10 mm). A border row can be used to finish the edges.
- Suitable over water-based underfloor heating when glued down and our Underfloor Heating Guide is followed.
4. Technical Summary: BS 8201 (for architects, specifiers and contractors)
A summary of good practice. It is not a copy of, or substitute for, the British Standard. The full standard, BS 8201:2011, is published by the British Standards Institution (BSI) at knowledge.bsigroup.com.
- Flatness: SR1 – no more than 3 mm under a 2 m straight edge.
- Moisture: concrete and screed below 65% RH by hygrometer (Annex A of BS 8201); 65–75% RH with an approved surface DPM; timber subfloors below 14% moisture content.
- Site conditions: building weathertight, wet trades dry, 15–25°C and 45–65% RH before, during and after installation.
- Acclimatisation: in packs in the room until stable (ESB recommends at least 72 hours).
- Methods: fully bonded (preferred for parquet, herringbone, wide boards and underfloor heating), secret nailed, or floating (engineered only).
- Expansion: continuous perimeter gap – ESB recommends at least 10 mm or 1.5 mm per metre of width, whichever is greater, with expansion breaks in large areas.
- Underfloor heating: floor surface never above 27°C; commission and run before installation (ESB recommends at least 14 days); bring temperatures back gradually (no more than 2°C per day).